# # AZ91E-T6, D.Goodenberger, MS Thesis, U.Iowa (superv. Prof.R.Stephens) # Room Temperature & Air Environment. Only the fully reversed tests shown here. # Ref: Thesis and SAE paper 930752 Mag. has very odd hyst. loops. # (Cyclic modulus on all short life tests is very low ~ 3600 to 4500) # Changed E from 6500 to 5500 to improve fit of cyclic S-e) # Changed to calculated Plastic Strain # #FileType= strain_life #DataType= raw #TIMEcol= 0 #NAME= MAGNESIUM #NAME= AZ91E-T6 #Stress_units= ksi #Su= 46.1 #Sy= 20.6 #E= 5500. #XK= 92.5 #XN= 0.249 #%RA= 12.8 #BHN= 0. #FractureStress= 51.6 #FractureStrain= 0.14 #NO. FAT. PTS.= 11 #Tot Strain 2Nf Stress Mean Plastic Strain Initial # Amp Amp Stress Amp Elastic Mod. 0.026 50. 39.7 0. 0.018782 5500. 0.020 138. 36.0 0. 0.013455 5500. 0.013 552. 32.1 0. 0.007164 5500. 0.013 518. 33.9 0. 0.006836 5500. 0.007 5086. 23.8 0. 0.002673 5500. 0.007 7142. 25.1 0. 0.002436 5500. 0.004 47060. 19.0 0. 0.000545 5500. 0.0040 57780. 19.1 0. 0.000527 5500. 0.003 1009020. 17.4 0. 0.0 5500. 0.003 494200. 17.1 0. 0.0 5500. 0.002 -2000000. 12.8 0. 0.0 5500. # #