# GKN_history, 128 Turning points (Peaks & Valleys)
##This is a history provided to FD+E by GKN in the 1970s. It was
#originally used to test Center Notched Plates. Kt=2.5,
#
# Material BS 4360-40B Steel
# Nominal Chem. appears to be 0.17C wt% 1.40Mn max, .045P max, .045 Smax
# Which is roughly a AISI or SAE 1522 (e.g. here )
# Experimental Plate Test Results:
# Test Level Test Life
# ABS(Nom. Stress Rg) (history repetitions)
# 69.0 ksi 450
# 51.5 2,206
# 90.5 65
# 44.8 4,425
# 39.6 9,849
# 39.6 (with -21.47 mean) 125,000 #runout
# 51.5 (with +21.47 mean) 1,126
#
#Numbers below: Max.Range= 100 Units (Thus max is +50, min is -50)
#
#BEGIN DATA
0
32.5
10
38.75
-23.75
13.75
-42.5
-20.625
-41.25
20
-38.75
40
5
44.375
-22.5
20
-40
-8.75
-40
41.25
-28.75
-8.75
-41.25
37.5
-22.5
-6.25
-38.75
25
-16.25
35
6.25
42.5
-37.5
33.75
-30
-6.25
-22.5
25
-37.5
-17.5
-50.
36.25
10.
46.25
-25
-8.75
-45.625
36.25
-26.25
18.75
-26.25
22.5
-28.75
33.75
-35
-12.5
-32.5
-12.5
-35
46.875
-31.25
-15
-45
-3.125
-46.25
-3.124
-39.375
-3.75
-38.75
37.5
6.25
38.75
5.
31.25
-40.
31.25
-29.375
21.25
5.
43.75
-37.5
25
-28.125
37.5
9.375
40.625
-43.75
14.375
-18.75
31.25
-33.75
31.25
-28.75
-12.5
-42.5
31.875
7.5
42.5
-33.75
-2.5
-38.75
37.5
-26.875
20.625
7.5
34.375
-39.375
-11.25
-39.375
-3.75
-27.5
35.625
-23.75
17.5
-28.75
41.25
-36.25
35
7.5
35
5
50
-50
25
0
30
-5
0
#